- Fe-Cr-Al Alloys
- Nickel-chromium Alloys
- Cn/Mn-Cu Alloys
- Cu-Ni Alloys
-
Precision Alloys
- Wire
- 1J330(1J30)
- 1J331(1J31)
- 1J332(1J32)
- 1J338(1J38)
- 1J350(1J50)
- 1J479(1J79)
- 1J485(1J85)
- 4J332(4J32)
- 4J332A(4J32A)
- 4J328(4j34)
- 4J329(4J29)
- 4J336(4J36)
- 4J342(4J42)
- 4J343(4J43)
- 4J352(4J49)
- 4J350(4J50)
- 6J415(6J15)
- 6J420(6J20)
- 6J422(6J22)
- 6J423(6J23)
- 6J424(6J24)
- 6J425(6J25)
- 6J426(6J26)
- 6J520(6J27)
- 6J525(6J28)
- Flat Wire
- 1J330(1J30)
- 1J331(1J31)
- 1J332(1J32)
- 1J338(1J38)
- 1J350(1J50)
- 1J479(1J79)
- 1J485(1J85)
- 4J332(4J32)
- 4J332A(4J32A)
- 4J328(4j34)
- 4J329(4J29)
- 4J336(4J36)
- 4J342(4J42)
- 4J343(4J43)
- 4J352(4J49)
- 4J350(4J50)
- 6J415(6J15)
- 6J420(6J20)
- 6J422(6J22)
- 6J423(6J23)
- 6J424(6J24)
- 6J425(6J25)
- 6J426(6J26)
- 6J520(6J27)
- 6J525(6J28)
- Flat Strip
- 1J330(1J30)
- 1J331(1J31)
- 1J332(1J32)
- 1J338(1J38)
- 1J350(1J50)
- 1J479(1J79)
- 1J485(1J85)
- 4J332(4J32)
- 4J332A(4J32A)
- 4J328(4j34)
- 4J329(4J29)
- 4J336(4J36)
- 4J342(4J42)
- 4J343(4J43)
- 4J352(4J49)
- 4J350(4J50)
- 6J415(6J15)
- 6J420(6J20)
- 6J422(6J22)
- 6J423(6J23)
- 6J424(6J24)
- 6J425(6J25)
- 6J426(6J26)
- 6J520(6J27)
- 6J525(6J28)
- Bar
- 1J330(1J30)
- 1J331(1J31)
- 1J332(1J32)
- 1J338(1J38)
- 1J350(1J50)
- 1J479(1J79)
- 1J485(1J85)
- 4J332(4J32)
- 4J332A(4J32A)
- 4J328(4j34)
- 4J329(4J29)
- 4J336(4J36)
- 4J342(4J42)
- 4J343(4J43)
- 4J352(4J49)
- 4J350(4J50)
- 6J415(6J15)
- 6J420(6J20)
- 6J422(6J22)
- 6J423(6J23)
- 6J424(6J24)
- 6J425(6J25)
- 6J426(6J26)
- 6J520(6J27)
- 6J525(6J28)
- Wire
- Ni-Al Alloys
- Pure Nickel Alloys
- Monel Alloys
- Hastelloy Alloys
- Inconel Alloys
- Incoloy Alloys
- Haynes Alloys
Monel Alloys Steel Bar monel K500
Overview
Monel Alloys Steel Bar monel K500 is a solid-solution alloy that can be hardened only by cold working. It has high strength and toughness over a wide temperature range and excellent resistance to many corrosive environments.
Alloy 400 is widely used in many fields, especially marine and chemical processing. Typical applications are valves and pumps; pump and propeller shafts; marine fixtures and fasteners; electrical and electronic components; springs; chemical processing equipment; gasoline and fresh water tanks; crude petroleum stills, process vessels and piping; boiler feedwater heaters and other heat exchangers; and deaerating heaters.
Limiting Chemical Composition, %
Nickel (plus Cobalt).................................................................................................................................................................63.0 min.
Carbon.....................................................................................................................................................................................0.30 max.
Manganese..............................................................................................................................................................................2.00 max.
Iron...........................................................................................................................................................................................2.50 max.
Sulfur......................................................................................................................................................................................0.024 max.
Silicon.......................................................................................................................................................................................0.50 max.
Copper..................................................................................................................................................................................28.00-34.00
Physical Constants
Density |
lb/in^3.............................................................................................0.318 |
g/cm^3.............................................................................................8.80 | |
Specific Heat |
Btu/lb•°F.........................................................................................0.105 |
J/kg•°C..............................................................................................440 | |
Melting Range |
°F............................................................................................2370-2460 |
°C...........................................................................................1300-1350 | |
Curie Temperature |
°F……...….....................................................................................….70-120 |
°C............…..................................................................................….21-49 | |
Modulus of Elasticity, 10^3 ksi |
Tension ............................................................................................26.0 |
Compression ...................................................................................26.0 | |
Torsion................................................................................................9.5 | |
Poisson’s Ratio................................................................................0.32 |
Mechanical properties
MONEL alloy 400 has excellent mechanical properties at subzero temperatures. Strength and hardness increase with only slight impairment of ductility or impact resistance.The alloy does not undergo a ductile-to-brittle transition even when cooled to the temperature of liquid hydrogen.
This is in marked contrast to many ferrous materials which are brittle at low temperatures despite their increased strength.
Tensile-properties
Nominal Room-Temperature Tensile Properties of MONEL Alloy 400 | |||||||
Form and Condition |
Tenslle Strength |
Yleld Strengt (0.2%Offset |
Eongation % |
Hardness |
|||
ksi |
MPa |
ksi |
MPa |
Brinel 3000-kg) |
Rockwell B |
||
Rod and Bar |
|||||||
Annealed |
75-90 |
517-620 |
25-50 |
172-345 |
60-35 |
110-149 |
60-80 |
Hot-Finished (except Hexagons over 21/8 inches and Angles) |
80-110 |
552-758 |
40-100 |
276-690 |
60-30 |
140-241 |
75-100 |
Hot-Finished Hexagons over 21/8 inches and Angles |
75-100 |
517-690 |
30-55 |
207-379 |
50-30 |
130-184 |
72-90 |
Cold-Drawn,Stress-Relieved |
84-120 |
579-827 |
55-100 |
379-690 |
40-22 |
160-225 |
85-20C |
Plate |
|||||||
Hot-Rolled,As-Rolled |
75-95 |
517-655 |
40-75 |
276-517 |
45-30 |
125-215 |
70-96 |
Hot-Rolled,Annealed |
70-85 |
482-586 |
28-50 |
193-345 |
50-35 |
110-140 |
60-76 |
Sheet |
|||||||
Annealed |
70-85 |
482-586 |
30-45 |
207-310 |
45-35 |
一 |
65-80 |
Cold-Rolled,Hard |
100-120 |
690-827 |
90-110 |
621-758 |
15-2 |
93 min. |
|
Strip,Cold-Rolled |
|||||||
Annealed |
70-85 |
482-586 |
25-45 |
172-310 |
55-35 |
一 |
68 max. |
Spring Tempe |
100-140 |
690-965 |
90-130 |
621-896 |
15-2 |
98 min. |
|
Tube and Pipe,Seamless |
|||||||
Cold-Drawn,Annealed |
70-85 |
482-586 |
25-45 |
172-310 |
50-35 |
一 |
75 max. |
Cold-Drawn,Stress-Relieved |
85-120 |
586-827 |
55-100 |
379-690 |
35-15 |
85-100 |
|
Heat-Exchanger,Annealed |
70-85 |
482-586 |
28-45 |
193-310 |
50-35 |
一 |
75 max. |
Heat-Exchanger,Stress-Relieved |
85-105 |
586-724 |
55-90 |
379-621 |
35-15 |
85-97 |
|
Hot-Extruded |
一 |
一 |
一 |
一 |
一 |
一 |
一 |
No.1 Temper (Annealed) |
85 max |
586 max |
30-45 |
207-310 |
45-30 |
73 max. |
|
No.2 Temper (Half-Hard |
85-105 |
586-724 |
55-80 |
379-552 |
30-10 |
一 |
75-97 |
No.3 Temper (Full-Hard |
110-130 |
758-896 |
90-110 |
621-758 |
10-3 |
95-27C |
|
Wire,Cold Drawn² |
|||||||
Annealed |
70-95 |
482-655 |
30-55 |
207-379 |
45-25 |
一 |
一 |
No.1 Temper |
85-100 |
586-690 |
50-75 |
345-517 |
30-20 |
||
Quarter-Hard |
95-120 |
655-827 |
65-95 |
448-655 |
25-15 |
一 |
一 |
Half-Hard |
110-135 |
758-931 |
85-120 |
586-827 |
15-8 |
||
Three-Quarter-Hard |
125-150 |
862-1034 |
100-135 |
690-931 |
8-5 |
||
Full-Hard--Spring Temper |
145-180 |
1000-124 |
125-170 |
862-1172 |
5-2 |
Corrosion Resistance
MONEL alloy 400 exhibits resistance to corrosion by many reducing media. It is also generally more resistant to attack by oxidizing media than higher copper alloys. This versatility makes alloy 400 suitable for service in a variety of environments.
Alloy 400 is widely used in marine applications. While alloy 400 products exhibit very low corrosion rates in flowing seawater, stagnant conditions have been shown to induce crevice and pitting corrosion. Alloy 400 is also resistant to stress corrosion cracking and pitting in most fresh and industrial waters.
MONEL alloy 400 offers exceptional resistance to hydrofluoric acid in all concentrations up to the boiling point. It is perhaps the most resistant of all commonly used engineering alloys. Alloy 400 is also resistant to many forms of sulfuric and hydrochloric acids under reducing conditions.
Heat Treatment
1.solid solution treatment
Heating: The monel K500 alloy is heated to a range of 980 °C to 1050 °C, and kept for a period of time, so that the various elements in the alloy are fully dissolved. This process usually needs to be carried out within a certain time frame so that the elements in the alloy can be fully diffused and evenly distributed. The specific heating time depends on the thickness of the alloy and the performance of the heating equipment.
Insulation: At the heating temperature, the alloy is kept for a certain time to ensure that the elements inside are completely dissolved and a uniform distribution is achieved. The holding time is usually 1 to 4 hours, depending on the composition of the alloy and the heating temperature.
Cooling: After the solution treatment is complete, the alloy needs to be cooled quickly to fix its tissue. Common cooling methods include water quenching or air cooling. The cooling speed will affect the properties of the alloy, so it is necessary to control the cooling speed to avoid excessive thermal stress.
2. Aging treatment
The purpose of aging treatment after solution treatment is to precipitate the phase in the alloy again to improve its mechanical properties.
The temperature of aging treatment is usually low, generally between 500 °C and 650 °C. The processing time varies depending on the desired properties and the composition of the alloy, usually ranging from tens to hundreds of hours. This process can be carried out in the air, or in a specific atmosphere or vacuum environment.
Through this heat treatment process, Monel alloy 400 alloy can obtain better corrosion resistance and high temperature strength. At the same time, attention should also be paid to controlling the various parameters of the heat treatment to obtain the best performance.
Available Forms
We provide you with a variety of product forms, including but not limited to
● Strip & Foil
● Round Wire &Flat Wire
● Bar & Rod
● Electrothermal Strip
● Flange & Ring
● Wire & Welding
● Reststance Wire
● Electric Alloy Wire
● Electric Furnace Bar
● Customize
description2